1.Molecular formula:
-{(CH2CF2)0.8--[CF(CF3)CF2]0.2}n-
2.Properties:
- Good heat
resistance,solvent-resistance and excellent oil -resistance;
- Good physical and
mechanical properties,good electrical insulation and anti-radiation properties;
- Working under 250oC
for long period,working at 300oC for short period;
- Low-temperature
resistance not bad.Glass-transition temperature -17oC. Brittle point -40oC~-55oC
;
- Not good resistance
to low M.W.ketones,esters,some ethers,anhydrous ammonia and active amines.
3.Applications:
Wildly used in
aviation,automobile,petroleum,and chemical industries,mainly for sealing purpose.
Especially good in the field of requiring heat-resistance and or
oil-resistance.Usually be made into "O" sealing rings,"V"sealing
rings,gasket,sealing bowl with metal bone.Suitable for both static and dynamic sealing of
hydraulic and lubricating systems.
4.Storage:
In shady cool and dry place.
Transportation
notes: Avoiding heating,moistening and exposing to the sun in
transportation. Non-hazardous chemicals.
5.Typical properties (Appendix
1. Grade classification by viscosity range - Appendix
2. Fluids Resistance Comparation )
|
BRAND |
FPM 2601 |
FPM 2602 |
FPM 2603 |
FPM 2604 |
Gum (before vulcanizing) |
Specific Gravity |
1.80 ~ 1.84 |
Nominal Mooney Viscosity,
ML121oC 1+10 |
20 ~ 40 |
50 ~ 60 |
70 ~ 100 |
110 ~ 180 |
Fluorine Content |
around 66 % |
Moisture Content |
max. 0.5% |
Vulcanized Elastomer
(without carbon black) |
Tensile Strength at Break,
MPa (before aging) |
----- |
min. 6.37 |
min. 7.50 |
min. 8.50 |
Tensile Strength at Break,
MPa (after aging) |
min. 160 |
min. 160 |
min. 150 |
min. 150 |
Elongation at Break, %
(before aging) |
min. 150 |
min. 150 |
min. 150 |
min. 150 |
Elongation at Break, %
(after aging) |
---- |
---- |
min. 120 |
min. 120 |
Oil Resistance, % (weight
increasing at 200oC X 24hr) |
max. 6 |
max. 6 |
max. 6 |
max. 6 |
Compression Set, % |
---- |
max. 55 |
max. 55 |
---- |
- APPENDIX
1. Grade Classification by
viscosity
|
Grade Name |
Mooney
Range |
Grade Name |
Mooney
Range |
FPM 2601 |
2601 A |
20 +- 10 |
FPM 2603 |
2603 A |
70 +- 10 |
2601 B |
30 +- 10 |
2603 B |
80 +- 10 |
2601 C |
40 +- 10 |
2603 C |
90 +- 10 |
FPM 2602 |
2602 A |
50 +- 10 |
2603 D |
100 +- 10 |
2602 B |
60 +- 10 |
FPM 2604 |
2604 A |
110 +- 10 |
--- |
--- |
2604 B |
140 +- 20 |
--- |
--- |
2604 C |
180 +- 20 |
- APPENDIX
2. Fluids Resistance Comparation
(Note: Red oil
i.e. campyhor oil)
|
Chemical Environment |
2# Fluoroelastomer
(copolymer) |
3# Fluoroelastomer
(terpolymer) |
RP-1 Kerosene
@ 200oCX24hr |
Weight Increasing Rate |
4.6 % |
4.4 % |
Volume Increasing Rate |
11.4 % |
11.8 % |
12# Red Oil
@ 200oCX24hr |
Weight Increasing Rate |
/ |
2.5 % |
Volume Increasing Rate |
/ |
6.1 % |
4109# Diester Oil
@ 200oCX24hr |
Weight Increasing Rate |
9.5 % |
4.7 % |
Volume Increasing Rate |
19.5 % |
9.7 % |
4104# Diester Oil
@ 130oCX24hr |
Weight Increasing Rate |
/ |
2.2 % |
Volume Increasing Rate |
/ |
5.1% |
10# Red Oil
@ 150oCX24hr |
Weight Increasing Rate |
1.1 % |
/ |
Volume Increasing Rate |
2.5 % |
/ |
8# Red Oil
@ 175oCX24hr |
Weight Increasing Rate |
/ |
1.1 % |
Volume Increasing Rate |
/ |
5.1 % |
|